> Sag
Features Causes Controlling Measures
On the low-lying part of coated surface, there appear sags and uneven film, which forms the tear-like marks and even curtain-like ones.    The viscosity of the paint is too low and film too thick Take reasonable control of the viscosity of the paint and the thickness of the film
The high temperature in the working place and slow drying time of the paint cause the film to run. Ensure good ventilation and choose the fast-dry paints
The nozzle of airbrush has been opened too widely Adjust the span of the airbrush nozzle
The coated surface is so uneven as to accumulate too much paint in its low-lying area Polish the surface as smooth as possible
The pressure from the air compressor is not stable and the distance between the airbrush and the coated surface not consistent. Adjust the air pressure to 0.4~0.6 MPQ
Due to the fast/slow-volatized solvent used Use the matching solvent to different paints, make sure the volatizing speed matches with the drying time of the paint
The paint is of too viscosity and the solvent volatizes too fast Adjust the viscosity of the paint with matching solvent
 

 